The effects of Co addition on the mechanical and microstructural properties of the matrix material of a Fe-based marble cutting tool
Access
info:eu-repo/semantics/openAccessDate
2016Access
info:eu-repo/semantics/openAccessMetadata
Show full item recordAbstract
In this study, four different kinds of marble cutting matrices with a base composition of Fe-Cu-Sn and with variable amounts of Co powder were produced. For compaction, hot sintering process was carried out at 850 degrees C under 35 MPa for 4 min. The mechanical and microstructural properties of the matrix materials were determined using SEM with EDS, three-point bending test, density and hardness measurement techniques. The addition of Co powders to the matrix and the subsequent hot sintering process affected the mechanical and microstructural properties of the cutting tool, such as hardness, total elongation, % porosity and phase distribution.